有變化,尤其性能也會(huì)比較穩(wěn)定。性能測(cè)試標(biāo)準(zhǔn)PC原料原料+1%FR100MBMF1(g/10min)ASTM D-9558.748.98拉伸強(qiáng)度(MPa)ASTM D-63861.562.68斷裂伸長率ASTM D-638208.25214.68彎曲強(qiáng)度(MPa)ASTM D-790101.89103.96彎曲模量(MPa)ASTM D-7902180.282285.76沖擊強(qiáng)度ASTM D-25687.7389.79阻燃性UL94 3.2mmHBV0玻璃化轉(zhuǎn)變溫度151.19152.63透光率(%)86.3985.99加工指南直接擠出造?;蛘咦⑺苤屑尤肜砘再|(zhì)Perkin-Elmcr熱分析(10℃/分,N2)失重% 溫度℃1 347.35 39710 41650 44690 517保存陰涼處儲(chǔ)存,保質(zhì)期一年包裝25公斤牛皮紙袋包裝